A field guide to galvanizing defects
Most rejected galvanizing can be traced to one step of the process. A table you can use on the inspection bench: what you see, the usual causes and where to fix it.
When a load comes out of the kettle with a fault, the instinct is to blame the zinc. In our experience the kettle is rarely the root cause. Most defects start earlier, in fabrication, degreasing, pickling, fluxing or drying, and a few come later, in quenching, handling and storage. Knowing which step to look at saves days of argument and a lot of re-galvanizing.
The table below covers the faults we are asked about most often. The articles linked at the end go into the main ones in detail.
| What you see | Usual causes | Where to fix it |
|---|---|---|
| Bare or uncoated spots | Oil, paint, marker or weld slag left on the steel; scale not pickled off; weak or dirty flux; flux dried out or burnt | Fabrication, degreasing, pickling, fluxing, drying |
| Ash inclusions: dull grey, powdery lumps | Zinc ash dragged up as the work leaves the bath; surface not skimmed at the withdrawal point | Kettle practice |
| Dross pimples: small hard bumps | Dross stirred up from the kettle floor; work dipped too deep; too much iron carried in from the flux | Kettle practice, flux control |
| Flux inclusions: black or brown spots | Flux too thick or wet; flux salts trapped under the zinc | Fluxing and drying |
| Runs, drips and spikes | Withdrawal too fast; zinc too cold; no drain holes; poor hanging angle | Kettle practice, design, jigging |
| Thick, dull grey coating | Reactive steel (silicon and phosphorus); slow cooling of heavy sections | Steel selection, bath alloying, immersion time |
| Flaking or peeling | Very thick, brittle alloy layers on reactive steel; long immersion; rough handling | Steel selection, immersion time, handling |
| Rough coating | Over-pickling; reactive steel; dross; uneven surface on the steel | Pickling, steel selection |
| Rust stains weeping from joints | Acid trapped in overlapping surfaces or narrow gaps | Design: seal-weld or open the gap |
| White rust (wet storage stain) | Fresh galvanizing kept wet and close-packed without air | Passivation, stacking and storage |
| Distortion | Thin and thick parts in one piece; asymmetric sections; locked-in welding stress | Design and dipping practice |
Is it a defect or only how it looks?
ISO 1461 and IS 4759 judge a coating mainly on two things: that it is continuous, and that it meets the minimum thickness for the steel thickness. A dull grey finish on reactive steel, or slight roughness, protects as well as a bright finish of the same thickness. Bare spots, lumps that stop the part being used, flux residues and inclusions that hide uncoated steel are real defects. Agree the standard and any special finish requirement with the customer before the order, not after the load comes out.