Coating defects

Bare spots: causes and cures

An uncoated spot is the one defect every customer rejects. Almost all of them are made before the steel reaches the kettle.

Zinc only reacts with clean steel. Anywhere the surface is still covered with oil, paint, scale, slag or a broken flux film, the zinc runs off and leaves a bare spot. So the first question for any bare spot is: what was on that area of the steel when it went into the zinc?

Read the shape of the spot

Shape and placeMost likely cause
Sharp-edged patch, often with writing or a linePaint, marker pen, crayon or sticker that degreasing cannot remove
Next to weldsWeld slag, spatter or anti-spatter spray
Smooth, rounded areas, often on the top sideOil or grease not removed: weak or cold degreaser, or too short a time
Dark grey scale still visible under the edgesMill scale or rust not pickled off
Many small spots over the whole pieceWeak, dirty or wrongly balanced flux; flux burnt off in an overheated dryer
Inside corners and pockets, mostly on the top sideTrapped air or gas: no vent hole
Marks where the piece hungContact with the jig, wire or another piece

Fixes, step by step

  1. Fabrication: ask the fabricator to avoid oil paint and marker on surfaces to be galvanized, to use water-based marking, and to grind or blast weld slag. Silicone anti-spatter sprays do not come off in pretreatment.
  2. Degreasing: keep the bath at its working temperature, check its strength every shift and skim the oil. A water-break test after rinsing shows whether the surface is clean: water should sheet, not bead.
  3. Pickling: pickle until the surface is uniformly grey with no scale, and do not rely on time alone. Acid that is weak or loaded with iron pickles slowly.
  4. Fluxing: hold flux strength, ratio, pH and iron in range, and keep the bath warm. A thin, even, dry film is the goal.
  5. Drying: dry fully, but do not overheat. Flux that is baked or burnt protects nothing.
  6. Design and hanging: vent every closed space, and hang the work so air can escape and zinc can reach every surface.

Repair or re-dip

ISO 1461 allows small bare areas to be repaired with zinc-rich paint, zinc thermal spray or zinc solder. The total must stay within 0.5 % of the surface and no single area over 10 cm². The 2009 edition asked for the repair to be at least 30 µm thicker than the local coating requirement; the 2022 edition asks for at least 100 µm unless agreed otherwise. Beyond those limits, strip and re-galvanize. See repairing galvanized steel.

Products in this article

More insights