Galvanizing practice

Dross in the kettle: where the iron comes from and how to take it out

Every kilogram of iron that reaches the zinc becomes dross. The chemistry, the three sources of iron, and a drossing routine that keeps bath and coating clean.

Dross is the price of iron, paid in zinc. Every kilogram of iron that reaches the bath ends up as dross on the kettle floor, and every kilogram of dross is mostly zinc you bought. Dross also spoils coatings when it is stirred up, as small hard pimples on the work. Controlling it means knowing where the iron comes from, and taking the dross out without taking zinc with it.

What dross is

Molten zinc at bath temperature can hold only a few hundredths of a per cent of iron in solution. Any more and the iron comes out as crystals of a zinc and iron compound, FeZn13, the zeta phase, about 6 per cent iron and 94 per cent zinc. The crystals are denser than liquid zinc, about 7.2 against 6.6 g/cm³, so they sink and collect on the floor as bottom dross.

The arithmetic is unforgiving. In the compound itself each kilogram of iron binds about 15 kg of zinc. The dross you lift out also carries liquid zinc trapped between the crystals, so in practice each kilogram of iron costs 20 to 25 kg of zinc. See where your zinc really goes.

When the bath carries more aluminium, part of the iron forms an iron and aluminium compound instead, which is lighter than zinc and floats as top dross. In batch galvanizing, with little aluminium in the bath, bottom dross is the one that matters.

Where the iron comes from

  1. The flux. Iron salts carried over from pickling, and iron dissolved from the steel in the flux tank, ride into the zinc on every piece. This is usually the largest source and the most controllable. See flux and your zinc bill.
  2. The steel. The coating forms as the steel surface dissolves into the zinc. Longer immersion, a hotter bath and reactive steel dissolve more.
  3. The kettle wall. The wall dissolves too: slowly where it is evenly heated, fast where it runs hot. A rising dross rate can be the first sign of a kettle in trouble.

Jigs, wire and hooks left hanging in the zinc, and work dropped into the bath, add iron as well.

Temperature and dross

Zinc dissolves more iron when it is hotter. A bath that swings up and down picks iron up on the way up and drops it as fresh, fine dross crystals on the way down. Fine crystals stay suspended longer and end up in the coating. A steady bath gives fewer, larger crystals that settle out. That is one more reason to hold the bath at 445 to 455 °C and to heat the kettle evenly.

A drossing routine

  • Let it settle. Dross settles while the bath is quiet. Drossing after a settling period, such as before the first shift, lifts more dross and less liquid zinc than drossing straight after heavy dipping.
  • Know the depth. Sound the dross layer with a rod and keep a clear margin between it and the lowest point of the deepest work. Drossing on a schedule beats drossing when pimples appear.
  • Use the right tool. A crane-suspended dross grab clears a large kettle quickly; the SHIVAS pneumatic grab takes a 400 kg bite in kettles 1.4 to 3.2 m deep (see it in 3D). Perforated ladles suit small kettles.
  • Drain before lifting out. Hold the full grab or ladle above the bath so the liquid zinc runs back.
  • Move slowly. Fast tool movement stirs fine dross back into suspension.
  • Weigh it. Record the dross removed each week and divide by the tonnes galvanized. That figure is the trend to watch.

Cutting the iron that comes in

SourceWhat to checkWhat to do
FluxIron in the flux, every dayRinse well after pickling, drain over the tanks, regenerate the flux continuously
SteelImmersion time; bath temperatureImmerse only as long as the steel needs; hold 445 to 455 °C
Kettle wallWall thermocouples; heat fluxEven heating; wall below about 480 °C; heat flux below about 18 to 20 kW/m²
Tools and jigsWhat is left in the bathTake wire, hooks and tools out of the zinc

Products in this article

More insights

All articles →